Freescale Semiconductor Ltd

Freescale Semiconductor — Technical Presentation

42 slides from Freescale Semiconductor's technical presentation

  1. Slide 1: Ceramic Ball Grid Array Packaging, Assembly & Reliability

    Ceramic Ball Grid Array Packaging, Assembly & Reliability Freescale Semiconductor 1

  2. Slide 2: Outline for Discussion

    Outline for Discussion • Why BGA???? • CBGA Introduction and Package Description • PC Board Design for CBGA • CBGA Assembly • Rework • Board-Level Solder Joint Reliability Freescale Semiconductor 2

  3. Slide 3: Why BGA?

    Why BGA????? • Advantages: – Higher Surface Mount Assembly Yield. » Coarse Pitches Compared to Fine Pitch Leaded. » Self-Centering. » Not Easily Susceptible to Handling Damage. – High I/O Density and High Pin Count Capability. – “Drop-In” Multi-Chip Capability. – Potentially Better Electrical and Th

  4. Slide 4: BGA Assembly Yields

    BGA Assembly Yields (As Reported by IBM and Compaq) 200 IBM Data on CBGA COMPAQ Data 150 .5 mm Pitch QFP on PBGA (Collapsing Ball) DPPMj* .65 mm Pitch QFP 100 1.27 mm Pitch CBGA 85 85 80 60 50 48 20 30 15 15 12 < 0.5 (COMPAQ ) <5 5 1 2 1991 1992 1993 1994 Year * DPPMj = Defective Joints Per Million

  5. Slide 5: CBGA Construction

    CBGA Construction 97Pb/3Sn C4* Joint Silicon Die Alumina (Al2O3) Ceramic Epoxy Substrate Underfill 0.89 mm Solder Ball 1.27 mm Pitch for 1.27 mm Pitch 10Sn/90Pb 63Sn/37Pb Solder Solder Balls Ball to Substrate Attach C4 = Controlled Collapse Chip Connection (Evaporated 97Pb/3Sn Bump) Freescale Semico

  6. Slide 6: CBGA Construction (Cont.)

    CBGA Construction (Cont.) • 304 Pin C4*/CBGA (Motorola MPC106 PCI Bridge Chip) Underfill 21 mm Silicon Die Ceramic Substrate 25 mm * C4 = IBM Developed Controlled Collapse Chip Conne Freescale Semiconductor 6

  7. Slide 7: CBGA Construction (Cont.)

    CBGA Construction (Cont.) •SEM Micrograph of Board-Mounted CBGA Substrate (No Chip) Showing Substrate Circuitry. Freescale Semiconductor 7

  8. Slide 8: CBGA Solder Balls

    CBGA Solder Balls 0.89 mm Diameter 90% Pb and 10% Sn (by Weight) “High CBGA Substrate Melt” Solder Ball Held to CBGA Substrate and Motherboard with Eutectic (63Sn/37Pb) Solder. Typically 0.89 to 0.94 mm Eutectic Solder Applied to the Motherboard Before Reflow. Must Have Minimum Eutectic Solder Mothe

  9. Slide 9: Motorola Products in CBGA

    Motorola Products in CBGA Body Pin Pitch Array Comments/Products Size Count 14 x 22 119 and 1.27 7 x 17 Fast SRAMs 153 9 x 17 21 255 1.27 16 x 16 60X PowerPC™ products. 21 x 25 303 1.27 16 x 19 MPC105 and 106 PCI Bridge chips. 25 360 1.27 19 x19 7XX and 7410 PowerPC™ products. 29 483 1.27 22 x 22 74

  10. Slide 10: Example CBGA Case Outline Drawings: 119, 360 and 483 Pin CBGAs

    Example CBGA Case Outline Drawings: 119, 360 and 483 Pin CBGAs Freescale Semiconductor 10

  11. Slide 11: Motorola 119 Pin, 14x22 mm CBGA Case Outline Drawing

    Motorola 119 Pin, 14x22 mm CBGA Case Outline Drawing Note: This is an uncontrolled copy Freescale Semiconductor 11

  12. Slide 12: Motorola 360 Pin, 25 mm CBGA Case Outline Drawing

    Motorola 360 Pin, 25 mm CBGA Case Outline Drawing Note: This is an uncontrolled copy Freescale Semiconductor 12

  13. Slide 13: Motorola 483 Pin, 29 mm CBGA Case Outline Drawing

    Motorola 483 Pin, 29 mm CBGA Case Outline Drawing Note: This is an uncontrolled copy Freescale Semiconductor 13

  14. Slide 14: Incoming PCB Requirements for CBGA

    Incoming PCB Requirements for CBGA • Solder Pad Metal Finish Options – HAL or HASL (Hot Air Solder Leveled). – Entek Plus™ (from Enthone) or Other Organic Coatings. – Both Used Successfully with CBGA. • Board Flatness – Planarity Within Industry (i.e., IPC) Standards Is Fine. – CBGA Typically More F

  15. Slide 15: Stencil Printing Solder Paste

    Stencil Printing Solder Paste • Nominal CBGA Solder Paste Volume Needs to Be 7,000 Mils3. Minimum Volume of 4,800 Mils3. – 7.5 Mil Stencil With 34 Mil Apertures Accomplishes This. • Stencil Thickness Can Be From 5 to 14+ Mils Thick to Acheive This. • May Want to Make Stencil Openings the Same Size A

  16. Slide 16: CBGA Solder Paste Stencil Thickness Versus Aperture Diameter Table

    CBGA Solder Paste Stencil Thickness Versus Aperture Diameter Table (Use to Achieve Nominal 7,000 mils3 or Minimum 4,800 mils3 Solder Paste Volume) Freescale Semiconductor 16

  17. Slide 17: CBGA NSMD Motherboard Solder Pad Geometry

    CBGA NSMD Motherboard Solder Pad Geometry • Recommended Non-Soldermask Defined (NSMD) Pad Dimensions. – 0.72 mm solder pad diameter. – Minimum solder paste volume of 4,800 mils3 (0.079 mm3) per pad. – Surface finish may be any consistently solderable surface such as organic solderability protectant

  18. Slide 18: BGA Placement

    BGA Placement • Most Newer Pick and Place Equipment Have Upward Looking Vision Systems That Can Recognize BGA. – Most Vendors of Older Equipment Have Retrofits Available. • Alignment Can Be From All Balls, Package Body or Perimeter Row of Balls Only. • No Vision Required for BGA With Mechanical Cent

  19. Slide 19: Reflow Guidelines for BGA

    Reflow Guidelines for BGA • Follow Guidelines Recommended by Solder Paste Supplier. – Flux Requirements Must Be Met for Best Solderability. • Recommended Profile: 210-215°C Peak, ≥75 Seconds Above 183° C (or Any Standard Surface Mount Reflow Profile). • Temperature Profile Should Be Carefully Charac

  20. Slide 20: Profiling Furnace for BGA

    Profiling Furnace for BGA • Profile Board Must Be Fully Populated to Simulate Thermal Load of the Production Board. • Reflow Profile Board to Keep All Parts in Place. – Guess at a Profile. Start Low and Increase Temperature Until High Mass Parts Solder. • Select Components to Monitor. – Highest Mass

  21. Slide 21: Thermocouple Attachment Method for CBGA

    Thermocouple Attachment Method for CBGA • Before Soldering Parts on Profile Board: – Drill Hole in PC Board (Just Large Enough for Thermocouple Wire) Through a Solder Pad in the Center of the CBGA Site. • Assemble All Components and Reflow by Normal Method. • Using Same Drill Bit, Drill Into Ball, A

  22. Slide 22: Thermocouple Attachment Method for CBGA (Cont.)

    Thermocouple Attachment Method for CBGA (Cont.) • Thermocouple Attachment Inside CBGA Solder Ball Freescale Semiconductor 22

  23. Slide 23: Secondary Reflow of BGA in Wave Soldering

    Secondary Reflow of BGA in Wave Soldering • A Wave Solder Operation Is Often Required After Surface Mount Devices Have Been Soldered on the Board. • The Partial Re-Reflow of BGA Solder Joints in This Secondary Operation Must Be Avoided. – The Result Can Be Open BGA Solder Joints. • PBGAs Are Low The

  24. Slide 24: Avoiding Secondary Reflow Of BGA in Wave Soldering

    Avoiding Secondary Reflow Of BGA in Wave Soldering • Optimize Wave Solder Operation to Minimize BGA Temperature (As Measured Below the BGA). • Utilize Wave Solder Pallets to Block Solder From BGA Area. • Block Heat Transfer Through BGA Vias by Plugging Them or Tenting With Soldermask on Bottomside.

  25. Slide 25: Cleaning After Reflow; BGA Inspection

    Cleaning After Reflow • The Industry Is Moving to No-Clean Fluxes, but Due to Large Pitch and High Standoff, Any Conventional Cleaning Process Can Typically Be Used. – Ensure That Spray Nozzles Direct Flow at an Angle to Potentially Clean Under the Part. BGA Inspection • External Solder Joints Can B

  26. Slide 26: BGA Assembly Yield - Top Ten Causes of BGA Assembly Defects

    BGA Assembly Yield - Top Ten Causes of BGA Assembly Defects • In No Particular Order: – Popcorning of Plastic BGA Parts Due to Not Following Out of Dry-Pack Requirements. Results in Shorting Balls. This Is a PBGA Issue Only Since CBGA Is Level I. – Poor Incoming Board Quality (Unsolderable Pads Due

  27. Slide 27: BGA Rework

    BGA Rework • Due to Lack of Solder Joint Visibility BGAs Are Often Falsely Blamed for Board Electrical Problems. – In Study Done by Compaq Computers (Suzanne Fauser, et al) 1 75% of All BGAs Removed From Production Boards During the Period of Study Were Found Have Been Incorrectly Removed Due to Ina

  28. Slide 28: BGA Component Removal in Rework

    BGA Component Removal in Rework • If the Board Is Thick With Internal Ground Planes: • Use Additional Localized Bottom Side Heat. • Preheat Entire Board to at Least 80°C (or Higher, As Permitted by Least Heat Tolerant Components Involved). –Elevating the Temperature of the Entire Board Will Reduce T

  29. Slide 29: Example of BGA Rework Nozzle With Exhaust

    Example of BGA Rework Nozzle With Exhaust (One Type of Patented Air-Vac Nozzle Shown) • Advantages: – Minimum Heating of Neighboring Parts. – Rapid Heating (Lower Rework Cycling Time). • Potential Issues: – Gradients Across Part May Make One Side Reflow First (Part Tilt). – Narrow Process Window (i.

  30. Slide 30: Examples of Non-Shell Type BGA Versus QFP Rework Nozzles

    Examples of Non-Shell Type BGA Versus QFP Rework Nozzles • Advantages: QFP Nozzles – Smaller Clearance (Note Slots for Perimeter Around Part Heating Only) Required. – One Nozzle Can Potentially Work for More Than One Body Size. BGA Nozzles (Note Pipes and – Wide Process Shrouds for Window. Directing

  31. Slide 31: Removing Excess Solder from Motherboard Solder Pads After BGA Removal

    Removing Excess Solder from Mother- board Solder Pads After BGA Removal • Redress of the Site without Damaging Soldermask Required to Achieve Relatively Flat Pads. – CBGA Sites May May Have Solder That Has a Higher Liquidus Due to Higher Lead Content as of a Result of Dissolution from the Solder Bal

  32. Slide 32: Flux/Solder Paste Application in Rework

    Flux/Solder Paste Application in Rework • CBGA Requires Exact Volume of Solder Paste (4,800 Mils3 Minimum for 1.27 mm Pitch) to Be Reapplied. • Several Options for Reapplying Solder Paste. – Custom Mini-Stencil (Preferred). – Screen Solder Paste Directly Onto CBGA Component. – Dispense of Solder Pas

  33. Slide 33: Solder Paste Application in Rework

    Solder Paste Application in Rework • Mini-Stencil Required to Apply Paste for CBGA/CCGA and Leaded Part Rework (Optional for PBGA). Freescale Semiconductor 33

  34. Slide 34: Placing New Component on Site

    Placing New Component on Site • The Rework Station Should Have Good Look- Up/Look-Down Capability. – Either Video or Optical Vision. – Split Prism Optics to Simultaneously View the BGA Balls and the Footprint Is Helpful. • Once Again, High Placement Accuracy Not Required Due to the Self-Aligning Nat

  35. Slide 35: Rework Reflow; Cleaning After Rework

    Rework Reflow – Batch Oven Preheating (Typically 80°C) of Entire Board May Be Advisable, Especially With Large Multilayer Boards, to Prevent Board Warpage or Localized “Oil-Canning”. • Pre-Heat Temperature Cannot Exceed Rating of Least Heat Tolerant Part on the Board. – Characterize Temperatures to

  36. Slide 36: Summary of BGA Rework Process

    Summary of BGA Rework Process • The Rework Process Goal Is Joint Structure and Quality at Least As Good As the Initial Assembly. • Robust Initial Assembly Process Reduces the Need for Reworking BGA Packages. • Removing and Replacing a BGA Can Be Easier Than for a QFP Due to Self Alignment. –However,

  37. Slide 37: CBGA Construction Influence on Attachment Reliability

    CBGA Construction Influence on Attachment Reliability • For CBGA, Ceramic Substrate Mismatched to FR4/Glass PCB. • Causes Joints Farthest from the Center to Fail First (i.e., Greatest Distance from the Neutral Point or DNP) Ceramic Substrate (6.7 ppm/°C) Increasing DNP FR4/Glass PCB (15-21 ppm/°C) F

  38. Slide 38: Accelerated Thermal Cycling Conditions

    Accelerated Thermal Cycling Conditions • Accelerated Thermal Cycling (ATC) Performed on Mounted Daisy-Chain Packages to Obtain Failure Distributions. – Two Conditions Used Are 0 to 100°C (-48 cpd) & -40 to 125°C (24 cpd). – Testing Continues Until >50% Packages Exhibit at Least One Joint Fail. 140 1

  39. Slide 39: Motorola Board-Level Cycling Typical Test Board Configuration

    Motorola Board-Level Cycling Typical Test Board Configuration • Four Layer FR-4 Epoxy/Glass Test Board Used. • Simulated Half-Ounce Power and Ground Planes Included. • Nominal Solder Pad Diameters to Match the Device. – 0.0285” φ for 1.27 mm Pitch CBGA. • 4.50” x 7.25” x 0.062” Thick Board. • HASL a

  40. Slide 40: Freescale Semiconductor

    28.5 mil board pad diamter. 7.5 mil thick stencil. Double-sided used 35 mil stencil aperture opening. Single-sided used 28 mil stencil apertu Freescale Semiconductor 40

  41. Slide 41: 25 mm CBGA Board-Level Thermal Cycling Data on Log-Normal Plot

    25 mm CBGA Board-Level Thermal Cycling Data Plotted on a Log-Normal Plot (Both HASL and OSP Surface Finishes Tested) Freescale Semiconductor 41

  42. Slide 42: Comparison of Ceramic Substrate Technology

    Comparison of Ceramic Substrate Technology 1.27 mm Pitch Parts, 2 Cycles per Hour TC 99 % 360 - 25x25x1.2 L/rr Standard Ceramic P Substrate - HTCC 95 a 90 c k 80 a 70 g 60 e 50 s 40 30 \838 - 37.5x37.5x2.3 High Temp. Coefficient F of Expansion Ceramic 20 a Substrate - LTCC i 10 Dotted Line Assumes 8

Freescale Semiconductor — Technical Presentation on 6ix