Slide 1: Improved Accelerated Test Methods for Solar Panel Service Life Prediction
Improved Accelerated Test Methods for Solar Panel Service Life Prediction Chiou-Fu Wang, Ph.D. DuPont Photovoltaic Fluoromaterials (PVFM) SECI Workshop June 25, 2015
Slide 2: Environmental Stresses in the Field
Environmental Stresses in the Field • Photovoltaic modules are exposed to a wide range of stress conditions • Stresses operate on the module simultaneously and sequentially; synergistic effects are observed Copyright © DuPont 2015. All rights reserved
Slide 3: DuPont Collaborated with Downstream Stakeholders to Assess Solar Systems, Modules, and Materials
DuPont Collaborated with Downstream Stakeholders to Assess Solar Systems, Modules, and Materials in the Service Environment Subcomponent degradation mode pareto based on visual inspection Encapsulant, 4% Backsheet, 9% • Inspected >60 global installations (>200 MW & 1.5 Cell, 24% million modules) in
Slide 4: Backsheet is Critical to Protect a Solar Panel
Backsheet is Critical to Protect a Solar Panel Glass Encapsulant Side EVA Inner layer Cells Middle Layer EVA Outer Layer MOST CRITICAL Air side – this side is Backsheet exposed to the climate • Durable and reliable backsheet materials can enable longer lifetime, maximize power output and reduce risk
Slide 5: Risks Associated with Using Unproven Backsheet Materials
Risks Associated with Using Unproven Backsheet Materials • Backsheet degradation increases potential safety risks such as loss of electrical protection • Yellowing is a one sign of polymer degradation and an early indicator of performance issues • Cracking typically is associated with yellowing Copy
Slide 6: Outer Layer Backsheet Cracking and Yellowing
Outer Layer Backsheet Cracking and Yellowing Polyester-based backsheet • Years in service: 4 years • Location: Spain • 5,000 modules affected Copyright © DuPont 2015. All rights reserved
Slide 7: Yellowing of PET and Tedlar PVF-Based Backsheets (Field Data)
Yellowing of PET and Tedlar® PVF-Based Backsheets (Field Data) Field test: Measurement of backsheet color change after modules have been exposed for years in the field Results: Small color change for Tedlar®-based backsheets Significantly larger changes in b* for PET backsheets Tedlar® shows excepti
Slide 8: Aged Modules with PET-Based Backsheet Have Visible Degradation and Significantly Lower Power Output
Aged Modules with PET-Based Backsheet Have Visible Degradation and Significantly Lower Power Output 1. Standard PET 2. Standard PET 3. Tedlar® PVF film Defects Crack Yellowing Years in field 10 years 12 years 11 years Cell type Mono Poly Mono Wet leakage Pass Fail Pass b* (Yellowing) 9.0 14.2 2.7 Na
Slide 9: Shortcomings of Current IEC Qualification Tests
Shortcomings of Current IEC Qualification Tests • Current IEC qualification standards were designed to identify early failures due to module design; does not predict long-term durability • IEC qualification standards do not adequately address durability of materials to UV exposure and weathering and
Slide 10: UV Ageing in Standard is Far Below than the Environment
UV Ageing in Standard is Far Below than the Environment UV dosage under different climate conditions UV Dosage(kWh/m2) Desert Tropic Temperate Annual UV (kWh/m2) 91.7 78.5 56.9 25 year UV exposure to the back of 275 235 171 module Current Standard 15 - 100 Passing IEC certification test does not imp
Slide 11: PET-Based Backsheets Yellow, Lose % Elongation in UVA Exposures
PET-Based Backsheets Yellow, Lose % Elongation in UVA Exposures Yellowing Losing % Elongation UVA b* at 3000 hours UVA % Elongation at 3000 hours 7 300 6 250 5 200 % Elongation 4 0 hours 150 0 hours b* 3 3000 hours 3000 hours 100 2 50 1 0 0 TPT TPE HPET1 HPET2 TPT TPE HPET1 HPET2 Yellowing and loss
Slide 12: Recommended Sequential Tests
Recommended Sequential Tests Damp Heat UVA nX ) Thermal Cycling UVA ) Test: Backsheet or Modules Observe: Backsheet Yellowing, Cracking Damp Heat nX ) Thermal Cycling ) Test: Full-Size Laminates or Module Observe: Backsheet Cracking Xenon Water Spray Ageing Test: Backsheets: weathering (Xe), Observe
Slide 13: Tedlar film-based backsheets endures various climates for decades
Tedlar® film-based backsheets endures various climates for decades Gansu Beijing 27 years Power degradation: ~10% 1 Shanghai 3 Zhejiang Hainan 23 years 23 years Power degradation: 13.1% Power degradation: 6.1% 2 Only solar panels with reliable materials maximize power output and 25 or more year syst
Slide 14: Conclusions
Conclusions • Field inspections and fielded module analysis are key to fundamentally understand PV component performance and durability • There are risks associated with using unproven backsheet materials • Passing IEC certification test does not imply 25 year durability for backsheet materials. New
Slide 15: photovoltaics.dupont.com
photovoltaics.dupont.com Copyright © 2015 DuPont. All rights reserved. The DuPont Oval Logo, DuPont™, The miracles of science™, Materials Matter™, and all products denoted with ® or ™ are registered trademarks or trademarks of E.I. du Pont de Nemours and Company or its affiliates.